PRECISION IN MATERIAL. CLARITY IN SUPPLY.

PITTING RESISTANCE

PREN calculator and PREN number table

Enter chromium, molybdenum, tungsten and nitrogen to calculate PREN, or search for a grade to see its PREN range from the composition limits. PREN is used to compare stainless steels and nickel alloys by their resistance to pitting corrosion.

Chemical composition

Enter weight per cent; you can use the heat analysis from the mill certificate. Leave W = 0 for grades without tungsten.

PREN = Cr + 3.3 (Mo + 0.5 W) + 16 N

PREN value

34.622 + 3.3 × (3 + 0.5 × 0) + 16 × 0.17

Comparison

Result
34.6
304
17.5–21.1
316L
23.1–30.0
Duplex 2205
30.9–38.1
Super duplex 2507
37.7–46.5
904L
32.2–39.9
254 SMO
43.3
Alloy 625
51.2
PREN = 22 + 3.3 × (3 + 0.5 × 0) + 16 × 0.17 = 34.6

PREN number table

PREN of stainless steels, duplex grades and nickel alloys, calculated from the composition limits on each grade page (Cr, Mo, W and N in weight %).

Stainless steelsMaterial no. · PREN · Cr · Mo · N · W
GradeMaterial no.PRENCrMoNW
X2CrNi121.400310.5–13.010.5–12.5–0–0.03–
Custom 4551.454311.0–14.211–12.50–0.5––
4101.400611.5–13.511.5–13.5–––
410S1.400012.0–14.012–14–––
4201.402112.0–14.012–14–––
4201.402812.0–14.012–14–––
420F1.402912.0–15.512–13.50–0.6––
4161.400512.0–16.012–140–0.6––
4201.403412.5–14.512.5–14.5–––
Custom 4651.461413.5–16.611–12.50.75–1.25––
1.49231.492313.6–16.511–12.50.8–1.2––
15-5 PH1.454514.0–17.214–15.50–0.5––
4311.405715.0–17.015–17–––
17-4 PH1.454215.0–19.215–17.50–0.5––
X50CrMoV151.411615.7–18.114–15.50.5–0.8––
4301.401616.0–18.016–18–––
430Nb1.451116.0–18.016–18–––
17-7 PH1.456816.0–18.016–18–––
3011.431016.0–23.216–190–0.80–0.1–
1.41041.410416.2–19.515.5–17.50.2–0.6––
1.49381.493816.3–19.711–12.51.5–20.02–0.04–
Super 13Cr1.441516.5–21.811.5–13.51.5–2.5––
430F1.410516.7–20.016–180.2–0.6––
A-2861.498016.8–21.013.5–161–1.5––
1.45941.459417.0–21.613–151.2–2––
3211.454117.0–19.017–19–––
3471.455017.0–19.017–19–––
1.47421.474217.0–19.017–19–––
3051.430317.0–20.617–19–0–0.1–
3031.430517.0–20.617–19–0–0.1–
304Cu1.456717.0–20.617–19–0–0.1–
303Cu1.457017.0–22.617–190–0.60–0.1–
Nitronic 60–17.3–20.916–18–0.08–0.18–
440C1.412517.3–20.616–180.4–0.8––
4411.450917.5–18.517.5–18.5–––
3041.430117.5–21.117.5–19.5–0–0.1–
304L1.430717.5–21.117.5–19.5–0–0.1–
1.45301.453017.6–19.811.5–12.51.85–2.150–0.01–
1.45961.459617.6–19.911.5–12.51.85–2.150–0.02–
1.41221.412218.1–21.815.5–17.50.8–1.3––
13-8 Mo PH1.453418.9–21.712.25–13.252–2.50–0.01–
1.41231.412318.9–29.114–161–2.50.1–0.3–
4341.411319.0–22.616–180.9–1.4––
X15CrNiSi20-121.482819.0–22.819–21–0–0.11–
301LN1.431819.317.5–0.11–
1.48181.481819.9–23.218–20–0.12–0.2–
1.41121.411220.0–23.317–190.9–1.3––
15-7 Mo–20.6–25.914–162–3––
1.48351.483521.9–25.220–22–0.12–0.2–
309S1.483322.0–25.822–24–0–0.11–
1.41141.411422.5–27.817.5–19.51.5–2.5––
1.47621.476223.0–26.023–26–––
446 / X8Cr241.476323.0–27.623–26–0–0.1–
316Ti1.457123.1–26.816.5–18.52–2.5––
1.45781.457823.1–27.416.5–17.52–2.50–0.1–
3161.440123.1–28.416.5–18.52–2.50–0.1–
1.45981.459823.1–28.416.5–18.52–2.50–0.1–
316L1.440423.1–30.016.5–18.52–30–0.1–
3141.484124.0–27.824–26–0–0.11–
310S1.484524.0–27.824–26–0–0.11–
AM 355–24.4–28.815–162.5–3.250.07–0.13–
4441.452124.6182––
316L / 316LMo1.443525.3–30.517–192.5–30–0.1–
316LN1.442926.7–31.916.5–18.52.5–30.12–0.22–
316LVM1.444126.7–28.317.52.80–0.1–
317L1.443827.4–34.317.5–19.53–40–0.1–
4461.474928.4–33.026–29–0.15–0.25–
Nitronic 50–28.7–39.820.5–23.51.5–30.2–0.4–
S316751.447230.1–39.919.5–222–30.25–0.5–
317LMN1.443931.6–38.516.5–18.54–50.12–0.22–
310MoLN1.446632.2–36.824–262–2.50.1–0.16–
904L1.453932.2–39.919–214–50–0.15–
1.45651.456542.0–52.124–264–50.3–0.6–
Alloy 9261.452942.2–48.120–216–70.15–0.25–
254 SMO1.454743.3206.10.2–
1.46591.465949.2–58.623–255.5–6.50.35–0.51.5–2.5
1.46521.465253.3–60.223–257–80.45–0.55–
Duplex stainless steelsMaterial no. · PREN · Cr · Mo · N · W
GradeMaterial no.PRENCrMoNW
23041.436223.1–29.722–24.50.1–0.60.05–0.2–
Lean duplex 22021.406224.1–30.021.5–240–0.450.16–0.28–
21011.416224.5–28.621–220.1–0.80.2–0.25–
24041.466229.5–36.423–251–20.2–0.3–
3291.446030.1–37.825–281.3–20.05–0.2–
Duplex 22051.446230.9–38.121–232.5–3.50.1–0.22–
2551.450737.1–44.024–263–40.2–0.3–
Super duplex 25071.441037.7–46.524–263–4.50.24–0.35–
Super duplex S327601.450137.9–45.724–263–40.2–0.30.5–1
Nickel and cobalt alloysMaterial no. · PREN · Cr · Mo · N · W
GradeMaterial no.PRENCrMoNW
NiCr 60/152.486715.015–––
Alloy 3301.486415.0–17.015–17–––
Alloy X-7502.466915.515.5–––
Alloy 7512.469416.016–––
Alloy 6002.481616.016–––
Alloy DS1.486217.517.5–––
Nimonic 902.4632 / 2.496918.0–21.018–21–––
Alloy 8001.487619.0–23.019–23–––
Incoloy 800H1.495819.0–23.019–23–––
Incoloy 800HT1.495919.0–23.019–23–––
NiCr 80/202.486920.020–––
Nimonic 752.495120.020–––
Nimonic 80A2.495220.020–––
Alloy 6012.485123.023–––
Alloy 202.466025.6–30.919–212–3––
Alloy 9012.466227.5–37.111–145–7––
Alloy HR-1602.488028.0–33.0280–1–0–1
Alloy HR-1202.485428.2–32.3250–10.20–0.5
Alloy 7182.466828.9193––
Alloy 925–29.9203––
Incoloy 8252.485832.9233––
Waspaloy2.465433.2194.3––
Elgiloy2.471138.8–47.419–216–8––
Nimonic 2632.465039.1205.8––
Alloy 3332.460839.9253–3
L-6052.496444.820––15
Alloy 2302.473344.8–58.720–241–3–13–15
MP35N–48.7–55.719–219–10.5––
Alloy 6252.485651.221.59––
Alloy 6172.466351.7229––
Alloy G-302.460352.3305.5–2.5
Alloy X2.466552.7229–0.6
Hastelloy C-222.460270.52113.5–3
Alloy 6862.460673.4–86.419–2315–17–3–4.4
Alloy C-20002.467575.82316––
Hastelloy C-2762.481976.21616.5–3.5
Alloy B-22.461789.80.727––

What is PREN?

PREN (pitting resistance equivalent number) estimates the resistance of stainless steels and nickel alloys to pitting corrosion from their chemical composition. The formula comes from regression analysis of pitting and crevice corrosion tests in chloride solutions. A higher PREN goes with a higher critical pitting temperature (CPT).

PREN formula

The most common formula is PREN = %Cr + 3.3 × %Mo + 16 × %N. For grades containing tungsten, PREN = %Cr + 3.3 × (%Mo + 0.5 × %W) + 16 × %N is used, the form also used in ISO 15156 / NACE MR0175. With tungsten at 0 both give the same result, so the calculator uses the single formula.

The coefficients have no physical meaning; multiplying nitrogen by 16 does not make it 16 times as effective as chromium. Chromium, molybdenum and nitrogen are only partly interchangeable: each must be present at a minimum level.

How the PREN ranges in the table are calculated

Each grade’s PREN range is calculated from the composition limits on its grade page. The lower value uses the lower limits and the upper value the upper limits; an element with only a maximum (e.g. N ≤ 0.10 in 304L) counts as 0 in the lower value. Grades with a typical composition show a single value. For a specific heat, enter the actual analysis from the mill certificate into the calculator.

What PREN does not tell you

PREN is for ranking grades on one scale; on its own it does not predict how a material will behave in a given service. Temperature, chloride concentration, pH, crevice geometry, welding and the structure after heat treatment also affect resistance. Material selection should combine the relevant standard, test results and producer data.

What is pitting corrosion?

Pitting corrosion forms small but deep pits where the passive oxide film on stainless steel breaks down locally, typically under chloride ions. Most of the surface can look intact while pits grow through the wall. Seawater, saline environments and chloride-bearing process fluids are the main risks; molybdenum and nitrogen strengthen the film.

Frequently asked questions

How is PREN calculated?

PREN = %Cr + 3.3 × (%Mo + 0.5 × %W) + 16 × %N. For grades without tungsten W = 0 and the formula becomes %Cr + 3.3 × %Mo + 16 × %N. Values are in weight per cent.

What is the PREN of 316L?

For 1.4404 (316L), PREN is 23.1–30.0 from the EN 10088-3 composition limits. For 304 (1.4301), which has no molybdenum, it is 17.5–21.1.

What is the PREN of duplex 2205?

Duplex stainless steel 1.4462 (2205) has a PREN of 30.9–38.1 from its composition limits.

What PREN does super duplex have?

Super duplex grades are generally associated with a PREN above 40. For 1.4410 (2507) the range from the composition limits is 37.7–46.5; a heat at the lower limits can fall below 40, so specifications often state a minimum PREN separately.

What is the PREN of alloy 625?

From its typical composition, alloy 625 (2.4856) has a PREN of about 51.2. For 904L (1.4539) the range from the composition limits is 32.2–39.9.

Is a higher PREN always better?

No. PREN only compares resistance to pitting in chloride environments. Crevice corrosion, stress corrosion cracking, temperature and fabrication effects are not part of it.