316 better
- 304
- PREN 19.3
- 316
- PREN 25.7
More resistant to pitting; the difference shows in chlorides (salt water, marine air).
GRADE COMPARISON
Choose two or three grades to see the key differences in short sentences, ratings for corrosion, strength, machinability, welding and heat, tensile strength and hardness, and their W.Nr, AISI and UNS identities side by side. Chemical composition and physical properties (thermal expansion, conductivity, elasticity) open on request.
Stainless Steel · 1.4301 · S30400
Stainless Steel · 1.4401 · S31600
In-depth guide:304 vs 316 stainless steel: the differences
Estimated price: reference
No property where it leads
Estimated price: 75% dearer than 304
Equal: Strength · Machinability · Weldability · Heat resistance
316 better
More resistant to pitting; the difference shows in chlorides (salt water, marine air).
316 contains it, 304 does not
Improves resistance to pitting and crevice corrosion in chlorides.
More in 316
Stabilises the austenitic structure; improves toughness and formability.
More in 304
The element that makes steel stainless; more chromium means better corrosion resistance.
| Property | 304 | 316 |
|---|---|---|
| Corrosion | ||
| Strength | ||
| Machinability | ||
| Welding | ||
| Heat | ||
| Estimated price (vs 304) | reference | 75% dearer |
| Critical pitting temperature (ASTM G48 E) | 10 °C | 20 °C |
| Critical crevice temperature (ASTM G48 F) | <0 °C | <0 °C |
| Tensile strength (Rm) | 600 MPa | 570 MPa |
| Elongation | 55 % | 55 % |
| Hardness | 175 HB | 170 HB |
| Hardening | None (cold work) | None (cold work) |
| Magnetic | No | No |
| Material group | Stainless Steel | Stainless Steel |
| Material no. (W.Nr) | 1.4301 | 1.4401 |
| EN name | X5CrNi18-10 | X5CrNiMo17-12-2 |
| AISI | 304 | 316 |
| UNS | S30400 | S31600 |
| JIS | SUS304 | SUS316 |
| Density | 7.9 g/cm³ | 8 g/cm³ |
| PREN | 17.5–21.1 | 23.1–28.4 |
Ratings are the sourced values of the stainless steel grade chart. Rm, elongation and hardness: Outokumpu typical values at room temperature (HB hot-rolled, HRB cold-rolled product). Grade chart · Hardness conversion
Critical temperatures: Outokumpu Handbook (2013) Table 6:1 typical values; higher is better. They rank grades in a standard test and are not a service limit.
Estimated price: based on the 12-month average alloy surcharge; size, quantity and cutting are not included. How is the price set? · Request a quotation
| Element | 304 | 316 |
|---|---|---|
| C | ≤ 0.07 | ≤ 0.07 |
| Si | ≤ 1 | ≤ 1 |
| Mn | ≤ 2 | ≤ 2 |
| P | ≤ 0.045 | ≤ 0.045 |
| S | ≤ 0.03 | ≤ 0.03 |
| Cr | 17.5–19.5 | 16.5–18.5▼ |
| Ni | 8–10.5 | 10–13▲ |
| Mo | – | 2–2.5▲ |
| N | ≤ 0.1 | ≤ 0.1 |
Arrows mark elements markedly higher (▲) or lower (▼) than in grade 1. Values are the composition limits on the grade pages.
| Property | 304 | 316 |
|---|---|---|
| Modulus of elasticity, GPa | 200 | 200 |
| Thermal expansion 20–200 °C, 10⁻⁶/K | 16.5 | 16.5 |
| Thermal expansion 20–400 °C, 10⁻⁶/K | 17.5 | 17.5 |
| Thermal conductivity, W/(m·K) | 15 | 15 |
| Specific heat, J/(kg·K) | 500 | 500 |
| Electrical resistivity, Ω·mm²/m | 0.73 | 0.75 |
Source: EN 10088-1:2005 (Euro Inox tables of technical properties). Values are for the annealed condition at 20 °C. Thermal expansion calculator
The compositionally closest grades in the same material group. Choose one to open it as grade 2.
A close composition does not make a grade a direct substitute; check mechanical properties, the product standard and the specification.
When comparing two grades, start with the chemical composition: carbon affects strength and weldability, chromium and molybdenum corrosion resistance, nickel the austenitic structure and toughness, nitrogen strength and pitting resistance. The table places the composition limits from the grade pages side by side and marks the elements where grade 2 is markedly higher or lower. PREN expresses the difference in pitting resistance of stainless steels and nickel alloys as one number.
The list compares grades in the same material group by the average values of the main elements and ranks those with the smallest difference. Each alternative shows its most marked differences (e.g. “Mo +0.5”). This is compositional closeness, not equivalence: for substitution, check mechanical properties, the product standard, heat treatment condition and specification. For the names of the same grade in other standards, see the steel equivalent chart.
316 (1.4401) contains 2–2,5% molybdenum, while 304 (1.4301) has none. Molybdenum raises pitting resistance in chlorides: PREN is 17.5–21.1 for 304 and 23.1–28.4 for 316.
316L (1.4404) has at most 0,03% carbon, 316 (1.4401) at most 0,07%. The lower carbon reduces the risk of intergranular corrosion after welding.
As a super duplex, 2507 (1.4410) has more chromium (24–26%), molybdenum (3–4,5%) and nitrogen; 2205 (1.4462) has 21–23% Cr and 2,5–3,5% Mo. PREN is 30.9–38.1 for 2205 and 37.7–46.5 for 2507.
Both are copper-bearing precipitation hardening martensitic stainless steels. 17-4 PH (1.4542) has 15–17,5% Cr and 15-5 PH (1.4545) 14–15,5%; the lower delta-ferrite structure of 15-5 PH improves transverse toughness.