PRECISION IN MATERIAL. CLARITY IN SUPPLY.

GRADE COMPARISON

410 vs 420 stainless steel

410 and 420 are martensitic stainless steels hardened by heat treatment. The key difference is carbon: 0.08–0.15% in 410 and 0.16–0.25% in 420. More carbon gives 420 higher hardness and wear resistance, while 410 is tougher and somewhat easier to weld.

Grades to compare

GRADE 1

410

Stainless Steel · 1.4006 · S41000

GRADE 2

420

Stainless Steel · 1.4021 · S42000

Common comparisons:Duplex 2205 – 316L316Ti – 316L304 – 32117-4 PH – 316904L – 316L303 – 4164130 – 4140321 – 316304 – 310S254 SMO – 904L420 – 440C

Key differences

WHERE IT LEADS410
  • Machinability
  • Heat resistance
WHERE IT LEADS420
  • Strength

Equal: Corrosion resistance · Weldability

Property differences

Strength

420 better

410
300 MPa
420
500 MPa

Higher yield strength; carries the same load with a smaller section.

Machinability

410 better

410
3/5
420
2/5

Easier to machine, with higher cutting speeds and longer tool life.

Heat resistance

410 better

410
705 °C
420
620 °C

Works at higher temperature in air without scaling or embrittlement.

Main composition differences

Carbon (C)

More in 420

410
0.08–0.15
420
0.16–0.25

Raises strength and hardenability. Low carbon reduces the risk of intergranular corrosion after welding.

Chromium (Cr)

More in 420

410
11.5–13.5
420
12–14

The element that makes steel stainless; more chromium means better corrosion resistance.

Property410420
Corrosion1/5PREN 12.51/5PREN 13.0
Strength2/5300 MPa · plate, annealed3/5500 MPa · rod, annealed
Machinability3/5index 0.502/5steel type class
Welding1/5steel type class1/5steel type class
Heat2/5705 °C · continuous, in air2/5620 °C · continuous, in air
Tensile strength (Rm)560 MPa650 MPa
Elongation30 %20 %
Hardness––
HardeningQuench and temperQuench and temper
MagneticYesYes
Material groupStainless SteelStainless Steel
Material no. (W.Nr)1.40061.4021
EN nameX12Cr13X20Cr13 / X20Cr14
AISI410420
UNSS41000S42000
JISSUS410SUS420J1
Density7.7 g/cm³7.7 g/cm³
PREN11.5–13.512–14

Ratings are the sourced values of the stainless steel grade chart. Rm, elongation and hardness: Outokumpu typical values at room temperature (HB hot-rolled, HRB cold-rolled product). Grade chart · Hardness conversion

Chemical composition, %
Element410420
C0.08–0.150.16–0.25▲
Si≤ 1≤ 1
Mn≤ 1.5≤ 1.5
P≤ 0.04≤ 0.04
S≤ 0.03≤ 0.03
Cr11.5–13.512–14▲
Ni≤ 0.75–

Arrows mark elements markedly higher (▲) or lower (▼) than in grade 1. Values are the composition limits on the grade pages.

Physical properties · 20 °C
Property410420
Modulus of elasticity, GPa215215
Thermal expansion 20–200 °C, 10⁻⁶/K11.011.0
Thermal expansion 20–400 °C, 10⁻⁶/K12.012.0
Thermal conductivity, W/(m·K)3030
Specific heat, J/(kg·K)460460
Electrical resistivity, Ω·mm²/m0.600.60

Source: EN 10088-1:2005 (Euro Inox tables of technical properties). Values are for the annealed condition at 20 °C. Thermal expansion calculator

Alternatives to 410

The compositionally closest grades in the same material group. Choose one to open it as grade 2.

A close composition does not make a grade a direct substitute; check mechanical properties, the product standard and the specification.

410 – 420: C, Cr

Frequently asked questions

Is 420 harder than 410?

Yes. With the same heat treatment 420 reaches higher hardness, and even annealed its typical yield strength is higher (about 500 MPa against 300 MPa).

Where are 410 and 420 used?

410 is used for valve, pump and turbine parts and fasteners. 420 is preferred for blades, surgical instruments, moulds and wear-exposed shafts and parts.

Are 410 and 420 magnetic?

Yes. Both are martensitic and magnetic in every condition.