PRECISION IN MATERIAL. CLARITY IN SUPPLY.

GRADE COMPARISON

316Ti vs 316L stainless steel

316Ti and 316L share the same chromium-nickel-molybdenum base; they differ in how intergranular corrosion after welding is prevented. 316L limits carbon to 0.03%, while 316Ti binds carbon with titanium (Ti ≥ 5 × C). Corrosion resistance and annealed strength are practically the same.

Grades to compare

GRADE 1

316Ti

Stainless Steel · 1.4571 · S31635

GRADE 2

316L

Stainless Steel · 1.4404 · S31603

Common comparisons:Duplex 2205 – 316L304 – 32117-4 PH – 316410 – 420904L – 316L303 – 4164130 – 4140321 – 316304 – 310S254 SMO – 904L420 – 440C

Key differences

WHERE IT LEADS316Ti

No property where it leads

WHERE IT LEADS316L

No property where it leads

Equal: Corrosion resistance · Strength · Machinability · Weldability

Main composition differences

Carbon (C)

More in 316Ti

316Ti
≤ 0.08
316L
≤ 0.03

Raises strength and hardenability. Low carbon reduces the risk of intergranular corrosion after welding.

Nickel (Ni)

More in 316Ti

316Ti
10.5–13.5
316L
10–13

Stabilises the austenitic structure; improves toughness and formability.

Molybdenum (Mo)

More in 316L

316Ti
2–2.5
316L
2–3

Improves resistance to pitting and crevice corrosion in chlorides.

Property316Ti316L
Corrosion4/5PREN 24.94/5PREN 26.6
Strength1/5260 MPa · plate, annealed1/5260 MPa · plate, annealed
Machinability3/5steel type class3/5steel type class
Welding5/5steel type class5/5steel type class
Heat—4/5925 °C · continuous, in air
Critical pitting temperature (ASTM G48 E)–20 °C
Critical crevice temperature (ASTM G48 F)–<0 °C
Tensile strength (Rm)570 MPa570 MPa
Elongation50 %55 %
Hardness170 HB170 HB
HardeningNone (cold work)None (cold work)
MagneticNoNo
Material groupStainless SteelStainless Steel
Material no. (W.Nr)1.45711.4404
EN nameX6CrNiMoTi17-12-2X2CrNiMo17-12-2
AISI316Ti316L
UNSS31635S31603
JISSUS316TiSUS316L
Density8 g/cm³8 g/cm³
PREN23.1–26.823.1–30

Ratings are the sourced values of the stainless steel grade chart. Rm, elongation and hardness: Outokumpu typical values at room temperature (HB hot-rolled, HRB cold-rolled product). Grade chart · Hardness conversion

Critical temperatures: Outokumpu Handbook (2013) Table 6:1 typical values; higher is better. They rank grades in a standard test and are not a service limit.

Chemical composition, %
Element316Ti316L
C≤ 0.08≤ 0.03▼
Si≤ 1≤ 1
Mn≤ 2≤ 2
P≤ 0.045≤ 0.045
S≤ 0.03≤ 0.03
Cr16.5–18.516.5–18.5
Ni10.5–13.510–13▼
Mo2–2.52–3▲
N–≤ 0.1
Ti5 × C ≤ Ti ≤ 0.70–

Arrows mark elements markedly higher (▲) or lower (▼) than in grade 1. Values are the composition limits on the grade pages.

Physical properties · 20 °C
Property316Ti316L
Modulus of elasticity, GPa200200
Thermal expansion 20–200 °C, 10⁻⁶/K17.516.5
Thermal expansion 20–400 °C, 10⁻⁶/K18.517.5
Thermal conductivity, W/(m·K)1515
Specific heat, J/(kg·K)500500
Electrical resistivity, Ω·mm²/m0.750.75

Source: EN 10088-1:2005 (Euro Inox tables of technical properties). Values are for the annealed condition at 20 °C. Thermal expansion calculator

Alternatives to 316Ti

The compositionally closest grades in the same material group. Choose one to open it as grade 2.

A close composition does not make a grade a direct substitute; check mechanical properties, the product standard and the specification.

316Ti – 316L: C, Ni, Mo

Frequently asked questions

Can 316L replace 316Ti?

In most applications, yes: both resist intergranular corrosion after welding, and 1.4571 is often named as an alternative to 1.4404. If a specification or pressure equipment approval names one grade, the change needs approval.

Is 316Ti or 316L better?

Neither is better overall. 316L polishes better, since titanium carbonitrides in 316Ti can mark a polished surface. 316Ti is more common in German-origin specifications and parts working at elevated temperature.

Is 316Ti magnetic?

No. 316Ti and 316L are austenitic and not magnetic when annealed; slight magnetism can appear after cold forming.