Both are highly alloyed austenitic stainless steels. 254 SMO has about 6% molybdenum and 0.2% nitrogen, with a PREN around 43. 904L has 4–5% molybdenum, 24–26% nickel and 1.2–2% copper, with a PREN of 32–40. In the ASTM G48 E test the critical pitting temperature is 40 °C for 904L and 65 °C for 254 SMO (Outokumpu).

Grades to compare

GRADE 1

254 SMO

Stainless Steel · 1.4547 · S31254

GRADE 2

904L

Stainless Steel · 1.4539 · N08904

Common comparisons:Duplex 2205 – 316L316Ti – 316L304 – 32117-4 PH – 316410 – 420904L – 316L303 – 4164130 – 4140321 – 316304 – 310S420 – 440C

Key differences

WHERE IT LEADS254 SMO
  • Corrosion resistance
  • Strength
WHERE IT LEADS904L

No property where it leads

Equal: Machinability · Weldability

Property differences

Corrosion resistance

254 SMO better

254 SMO
PREN 43.3
904L
PREN 36.1

More resistant to pitting; the difference shows in chlorides (salt water, marine air).

Strength

254 SMO better

254 SMO
320 MPa
904L
260 MPa

Higher yield strength; carries the same load with a smaller section.

Main composition differences

Nickel (Ni)

More in 904L

254 SMO
18
904L
24–26

Stabilises the austenitic structure; improves toughness and formability.

Molybdenum (Mo)

More in 254 SMO

254 SMO
6.1
904L
4–5

Improves resistance to pitting and crevice corrosion in chlorides.

Nitrogen (N)

More in 254 SMO

254 SMO
0.2
904L
≤ 0.15

Raises strength and pitting resistance.

Property254 SMO904L
Corrosion5/5PREN 43.35/5PREN 36.1
Strength2/5320 MPa · plate, annealed1/5260 MPa · plate, annealed
Machinability1/5steel type class1/5steel type class
Welding3/5steel type class3/5steel type class
Heat—2/5550 °C · sigma phase limit
Critical pitting temperature (ASTM G48 E)65 °C40 °C
Critical crevice temperature (ASTM G48 F)35 °C10 °C
Tensile strength (Rm)680 MPa600 MPa
Elongation50 %50 %
Hardness160 HB155 HB
HardeningNone (cold work)None (cold work)
MagneticNoNo
Material groupStainless SteelStainless Steel
Material no. (W.Nr)1.45471.4539
EN nameX1CrNiMoCuN20-18-7X1NiCrMoCu25-20-5
AISI––
UNSS31254N08904
JISSUS312LSUS890L
Density8 g/cm³8 g/cm³
PREN43.332.2–39.9

Ratings are the sourced values of the stainless steel grade chart. Rm, elongation and hardness: Outokumpu typical values at room temperature (HB hot-rolled, HRB cold-rolled product). Grade chart · Hardness conversion

Critical temperatures: Outokumpu Handbook (2013) Table 6:1 typical values; higher is better. They rank grades in a standard test and are not a service limit.

Chemical composition, % · typical values for some grades
Element254 SMO904L
C≤ 0.02≤ 0.02
Si≤ 0.8≤ 0.7
Mn≤ 1≤ 2▲
P≤ 0.03≤ 0.03
S≤ 0.01≤ 0.01
Cr2019–21
Ni1824–26▲
Mo6.14–5▼
N0.2≤ 0.15▼
Cu0.71.2–2▲

Arrows mark elements markedly higher (▲) or lower (▼) than in grade 1. Values are the composition limits on the grade pages.

Physical properties · 20 °C
Property254 SMO904L
Modulus of elasticity, GPa195195
Thermal expansion 20–200 °C, 10⁻⁶/K17.016.1
Thermal expansion 20–400 °C, 10⁻⁶/K18.016.9
Thermal conductivity, W/(m·K)1412
Specific heat, J/(kg·K)500450
Electrical resistivity, Ω·mm²/m0.851.00

Source: EN 10088-1:2005 (Euro Inox tables of technical properties). Values are for the annealed condition at 20 °C. Thermal expansion calculator

Alternatives to 254 SMO

The compositionally closest grades in the same material group. Choose one to open it as grade 2.

A close composition does not make a grade a direct substitute; check mechanical properties, the product standard and the specification.

254 SMO – 904L: Mn, Ni, Mo, N, Cu

Frequently asked questions

Should I choose 254 SMO or 904L?

254 SMO leads in seawater and chlorides, especially where pitting and crevice corrosion are the risk. 904L offers good resistance in sulphuric acid and to stress corrosion cracking (Outokumpu).

Is 254 SMO or 904L more expensive?

From the last 12 months of alloy surcharges they are at about the same level, both more than three times 304. The exact price depends on size and quantity.

Are 254 SMO and 904L magnetic?

No. Both are austenitic and not magnetic when annealed.