What does the L mean?
L stands for low carbon. Under EN 10088-3, carbon is at most 0.07% in 304 / 1.4301 and 316 / 1.4401, and at most 0.030% in 304L / 1.4307 and 316L / 1.4404. Under ASTM the limit is 0.08% for 316 and 0.030% for 316L.
Chromium and nickel ranges are close within each pair. Molybdenum separates 316 from 304; the main difference between 304 and 304L, or between 316 and 316L, is carbon.
Why low carbon matters in welding
During welding, in the zone held in a certain temperature range, carbon can combine with chromium to form chromium carbides at grain boundaries. Chromium is depleted around these boundaries and the zone becomes susceptible to corrosion, called intergranular corrosion. The lower the carbon, the fewer such carbides form.
304L and 316L are therefore preferred for welded tanks, piping and heavy welded parts. For parts made by machining without welding, the difference is often not decisive.
304, 304L, 316 and 316L comparison table
The values below are from the EN 10088-3:2023 long-product table. PREN is an index used to rank corrosion resistance and is calculated from these limits.
| Property | 304 / 1.4301 | 304L / 1.4307 | 316 / 1.4401 | 316L / 1.4404 |
|---|---|---|---|---|
| EN name | X5CrNi18-10 | X2CrNi18-9 | X5CrNiMo17-12-2 | X2CrNiMo17-12-2 |
| Carbon (C), max % | 0.07 | 0.030 | 0.07 | 0.030 |
| Chromium (Cr), % | 17.5–19.5 | 17.5–19.5 | 16.5–18.5 | 16.5–18.5 |
| Nickel (Ni), % | 8.0–10.5 | 8.0–10.5 | 10.0–13.0 | 10.0–13.0 |
| Molybdenum (Mo), % | — | — | 2.0–2.5 | 2.0–3.0 |
| PREN | 17.5–21.1 | 17.5–21.1 | 23.1–28.4 | 23.1–30.0 |
Sources and technical details
Source: EN 10088-3:2023, Table 2, cast-analysis limits for long products. The composition of 1.4404 was changed in the 2023 edition (EN 10088-1:2023 foreword); material made to the 2014 edition has a molybdenum range of 2.0–2.5. The edition should be stated in the order.
PREN = Cr + 3.3 Mo + 16 N, with nitrogen at its 0.10% maximum. It is not a test result in a given environment.
EN 10088-3:2023 — official SIST preview (PDF) — Cast-analysis limits for long products; values follow Table 2 of the full text.
EN 10088-1:2023 — catalogue page and foreword — Changes from the previous edition, including the 1.4404 composition change.
Strength and dual-certified 304/304L, 316/316L
Lower carbon can reduce strength slightly. Under ASTM, the minimum yield and tensile values of 316L are therefore a little lower than those of 316.
Producers make material that meets both grades by keeping carbon below 0.030% and supporting strength with nitrogen. It is sold as dual-certified 316/316L or 304/304L: it meets the carbon limit of the L grade and the strength requirement of the other. The material certificate shows which requirements are met.
How can 316 and 316L be told apart?
The two grades cannot be told apart by appearance, magnet or density; the difference is in carbon only. Handheld XRF cannot measure carbon; carbon requires OES (optical emission spectrometry). On delivery, the cast analysis on the EN 10204 3.1 certificate shows the carbon content.
Which one to choose?
For welded fabrication 304L or 316L; for machined parts without welding, all four grades can be used. Dual-certified material meets both needs and is used as a single option in many applications. The choice between 304 and 316 depends on the chloride content of the environment rather than on welding.