HIGH TEMPERATURE
Heat-resistant stainless steels
Heat-resistant stainless steels are used in furnace internals, annealing boxes, burners and hot-gas equipment. Austenitic 309S, 310S and 314 and ferritic 1.4762 and 446 are well-known members.
Oxidation resistance and hot strength are separate properties
A thin sheet in a furnace guides gas; a hanger carries parts. For the sheet, oxidation resistance matters; for the hanger, carrying load while hot matters too. Hot metal under constant load can bend or stretch over time; this is creep, judged with separate data.
So one furnace may use several steels. Service temperature alone does not decide the choice; gas composition, thermal cycling and the load carried matter too.
Austenitic heat-resisting steels: 309S, 310S, 314, 153 MA and 253 MA
309S / 1.4833 and 310S / 1.4845 contain high chromium and nickel; chromium helps form a protective oxide layer. 314 / 1.4841 has more silicon, which adds surface protection in suitable oxidising gases. 1.4828, also sold as 309, is a separate steel with different silicon.
1.4835 (253 MA) and 1.4818 (153 MA) contain silicon, nitrogen and a small amount of cerium. Silicon and cerium support the protective layer and nitrogen adds strength; they are used in furnace parts that heat and cool repeatedly. Similar trade names do not mean the same composition.
Ferritic heat-resisting steels: 1.4742, 1.4762 and 446
1.4742 and 1.4762 contain chromium, aluminium and silicon; aluminium and silicon help protect the surface at temperature. 1.4762 has more chromium. Ferritic heat-resisting steels expand less than austenitic ones, which helps in long furnace parts and protection tubes. Being magnetic does not mean they are not heat resistant.
What does low expansion contribute?
Metal expands as it heats. In a long furnace part or broad plate, the change can be noticeable. Ferritic stainless steels expand less than common austenitic heat-resistant steels and generally conduct heat better. These differences matter between a part’s hotter and cooler regions.
Ferritic steels are attracted to a magnet. This does not mean they are not stainless or heat resistant; it is a feature of their steel family. The example below compares expansion on heating in two different steels.
| Freely expanding one-metre component | Mean coefficient over 20–600 °C (10⁻⁶/K) | Calculated expansion |
|---|---|---|
| 1.4742 — ferritic | 12.0 | About 6.96 mm |
| 309S / 1.4833 — austenitic | 18.0 | About 10.44 mm |
Sources and technical details
Both parts are 1000 mm long at 20 °C. The calculation assumes that every part reaches 600 °C and can expand without being held back by connections. Expansion = initial length × mean expansion coefficient × the 580 °C temperature difference.
The coefficients are guidance values from EN 10095:1999, Annex B, Table B.5. The calculated expansion does not set an assembly gap, dimensional tolerance or load capacity. Welded parts, or parts held back from moving, can behave differently. Less expansion alone does not give a furnace a longer life.
BSI — BS EN 10095:1999 — Annex B, Table B.5: mean linear expansion over 20–600 °C for 1.4742 and 1.4833. The expansion values are calculated examples, rather than measured component test results.
Where do 309S, 1.4835 and 1.4818 differ?
309S, 1.4835 and 1.4818 are austenitic heat-resistant stainless steels. They contain nickel; 1.4835 and 1.4818 also contain silicon, nitrogen and cerium. Their behaviour under hot loads and gas exposure differs from ferritic grades.
These steels can be used in similar furnace parts. A maximum temperature figure alone does not explain which is more suitable. Expansion on heating, surface resistance to hot gas and the load carried while hot are separate properties.
Do 1.4713 and 1.4763 belong to the same group?
1.4713 / X10CrAlSi7 is a ferritic heat-resistant steel containing 6–8% chromium. Aluminium and silicon help the surface resist oxidation in hot air. Its chromium content is below the generally accepted stainless steel threshold, so the catalogue places it among alloy steels. Resistance to hot air does not mean the same protection in wet conditions.
1.4763 / X8Cr24 contains 23–26% chromium and is a ferritic stainless steel. It is associated with the 446 family, but its composition differs from 1.4749 / X18CrN28. Use at similar temperatures does not make them the same material; the surrounding gas also matters.
| Grade | Chromium range | Principal distinction |
|---|---|---|
| 1.4713 | 6–8% | Heat-resistant alloy steel |
| 1.4763 | 23–26% | High-chromium ferritic stainless |
| 1.4749 | 26–29% | Different carbon and nitrogen limits |
Sources and technical details
Chromium amounts are percentages by mass. The 1.4713 and 1.4749 figures are cast-sample analysis limits from EN 10095:1999, Table 1. The 23–26% range for 1.4763 / X8Cr24 comes from Rodacciai’s wire-product document. The three rows do not share one source.
BSI — BS EN 10095:1999 — Table 1: chemistry for 1.4713 and 1.4749.
Rodacciai — Stainless Steel Solutions (PDF) — Printed p.58 / PDF p.59: X8Cr24 / 1.4763 wire entry and chromium range. Only that identity and range are used here; other processing and mechanical rows are not transferred.
309S: components exposed to hot gases
309S / 1.4833 is used for furnace internals, boxes for annealing metals and hot-gas baffles. It belongs to the austenitic stainless steel family and contains chromium and nickel. Chromium helps form a protective oxide layer at the surface.
Grade 1.4828 can also appear beside the name 309. It is a separate steel with different silicon content, not a second EN number for 1.4833.
1.4835: equipment experiencing changing temperatures
1.4835 / S30815 is also known by the trade name 253 MA. It contains silicon, nitrogen and a small amount of cerium. Silicon and cerium contribute to the protective surface layer, while nitrogen supports strength.
These properties are useful in furnace parts that repeatedly heat and cool. Uses include heating tubes, hot-material conveying equipment and furnace internals. Surface protection and carrying loads while hot can both matter in these parts.
1.4818: a separate steel known as 153 MA
1.4818 / S30415 is known by the trade name 153 MA. It contains silicon, nitrogen and cerium alongside chromium and nickel. It serves furnace and heating equipment where surface protection and strength while hot matter.
The names 153 MA and 253 MA are similar, but the steels are different. Their chromium and other element contents differ. Sheet and plate forms can serve broad-surfaced furnace internals.
Seeing the composition differences
The table below compares silicon, nitrogen and cerium contents in 309S, 153 MA and 253 MA. These elements have different roles in surface protection and strength while hot. Similar trade names do not mean the same composition.
| Material | Silicon (Si) | Nitrogen (N) | Cerium (Ce) |
|---|---|---|---|
| 309S / 1.4833 | ≤ 1.00 | ≤ 0.11 | No limit in this row |
| 153 MA / 1.4818 | 1.00–2.00 | 0.12–0.20 | 0.03–0.08 |
| 253 MA / 1.4835 | 1.40–2.50 | 0.12–0.20 | 0.03–0.08 |
Sources and technical details
Source: EN 10095:1999, Table 2. Values are cast-sample analysis limits given in mass percent. They are not a producer’s typical composition or measurements from a particular batch. The absence of a cerium limit for 309S does not mean cerium is absent.
Only three elements are shown; this does not replace the complete composition table. Matching nitrogen and cerium ranges do not make every property of 153 MA and 253 MA the same. These percentages cannot calculate a part’s life or load capacity.
BSI — BS EN 10095:1999 — Table 2: 1.4833, 1.4818 and 1.4835. Cast analysis and the product scope of the standard; not transferred to ASTM acceptance requirements.
Outokumpu — Therma brochure, 2017 (PDF) — pp.4 and 7–10: material identities, furnace applications and the distinction between oxidation and hot-load behaviour. The brochure’s typical chemistry is a different data type from the standard limits above.
Oxide scale and the silicon contribution in 314
An oxide layer forms on hot metal. When it stays attached and protective, it reduces direct contact between the gas and the metal beneath. If it flakes off, fresh metal can be exposed. Oxidation resistance describes how well this protection is maintained in hot conditions.
The chromium and nickel in 310S matter in hot use. Higher silicon in 314 provides an additional contribution in suitable oxidising gases: environments that oxidise the metal surface. Gas-flow sheets and furnace internals are uses where this can help.
Gases containing oxygen, carbon and sulfur can affect the surface differently. Heating and cooling, and deposits on the surface, also affect the protective layer. More silicon in 314 therefore does not mean a better result in every furnace.
| Grade | EN number | Silicon limit, % by mass |
|---|---|---|
| 310S | 1.4845 | ≤ 1.50 |
| 314 | 1.4841 | 1.50–2.50 |
Sources and technical details
Source: EN 10095:1999, Table 2; cast-sample analysis limits. These are not a producer’s typical composition or measurements from a particular batch. The ranges meet at 1.50%, so not every 314 part necessarily contains more silicon than every 310S part.
The silicon comparison supports the explanation of surface behaviour above. On its own, it cannot establish which component will last longer or what load it can carry.
BSI — BS EN 10095:1999 — Table 2: cast-analysis silicon limits for 1.4845 and 1.4841. Complete chemistry and other product requirements have their own scope.
Hot strength in supports, baskets and hangers
Hot metal can slowly bend or stretch under a sustained load. This is called creep. Temperature, the stress produced by the load and time affect the result. Baskets, supports and hangers need to retain their shape under load as well as protect their surfaces.
In a long bar between supports, the distance between supports and the position of the load affect bending. A shorter or differently supported bar can behave differently under the same load. The part’s thickness and shape therefore also matter.
Oxidation resistance and creep strength are different properties. A part with a well-protected surface still needs separate mechanical data for sustained loading. Those data need to match the temperature and duration involved.
How heating and cooling affect the component
As a furnace starts, stops or is loaded, the metal heats and cools, expanding and contracting. Thin areas can heat faster than thick ones. If connections prevent movement, additional stresses can build up locally. Part shape and connections therefore also affect its response to heating.
In a welded body, weld position and transitions between different thicknesses matter. Parent metal, weld metal and the connection heat and cool together. The way a joint accommodates this movement matters especially in thin sheet.
Manufacturing from sheet, plate and bar
Sheet and plate can become covers, sleeves, gas guides and welded bodies. Bar can be machined into hangers, shafts and connections. Cutting, bending and welding are common in sheet work; turning, drilling and milling shape bar parts.
Both steels can harden during forming; this is called work hardening. A later bend may need more force after cold bending. During machining, tool rubbing can also harden the layer encountered in the next cut. Stable cutting and effective cooling therefore matter.
In welded parts, surface oxides and manufacturing residues are addressed during final surface finishing. Cutting, forming and joining affect the finished part alongside its furnace duty.
304HCu and 310HCbN in boiler tubing
A furnace sheet and a boiler tube working under pressure have different jobs. 304HCu / S30432 and 310HCbN / S31042 are austenitic steels used for superheater and reheater tubes, which raise steam to higher temperatures. They are not the same materials as general 304 or 310S.
| Family / UNS | Distinguishing alloy approach | Associated scope |
|---|---|---|
| 304HCu / S30432 | Copper, niobium and nitrogen additions | ASTM/ASME A/SA-213; 1.4907 / VdTÜV 550 |
| 310HCbN / S31042 | High chromium-nickel; niobium and nitrogen | ASTM/ASME A/SA-213; 1.4952 / VdTÜV 546 |
Sources and technical details
The European designations are 1.4907 / X10CrNiCuNb18-9-3 and 1.4952 / X6CrNiNbN25-20. Producer documents also refer to VdTÜV 550 and 546 respectively. ASTM/ASME tube requirements and these European designations do not share every acceptance requirement. Additional features of particular commercial products do not apply to every product in these families.
Tubacex — Power Generation (PDF) — p.7: the producer’s tube-family table lists 30432 / 1.4907 / VdTÜV 550 and 310HCbN / 1.4952 / VdTÜV 546. These references do not make every standard’s acceptance requirements identical; commercial product properties retain their own scope.
Grades in this group
EN, AISI / SAE, UNS and JIS designations of the grades in this family. Designations from different systems do not always imply identical specification requirements.
| Grade / Alloy | EN / W.Nr. | AISI / SAE | UNS | JIS | Grade page |
|---|---|---|---|---|---|
| Heat-resistant stainless steels11 grades | |||||
| Grade page | |||||
| 309SHeat-resistant austenitic stainless | 1.4833X12CrNi23-13 / X7CrNi23-14 | 309S | S30908 | SUH309 | |
| X15CrNiSi20-12Heat resistant · Silicon bearing | 1.4828X15CrNiSi20-12 | — | — | — | |
| 310SHigh-temperature applications | 1.4845X8CrNi25-21 / X12CrNi25-21 | 310S | S31008 | SUS310S | |
| 314Heat-resistant grade | 1.4841X15CrNiSi25-21 / X15CrNiSi25-20 | 314 | S31400 | — | |
| 1.4835Heat-resistant · Nitrogen and silicon bearing | 1.4835X9CrNiSiNCE21-11-2 | — | S30815 | — | |
| 1.4818Heat-resistant · UNS S30415 | 1.4818X6CrNiSiNCe19-10 | — | S30415 | — | |
| 1.4742Chromium-aluminium-silicon · Ferritic | 1.4742X10CrAlSi18 / X10CrAl18 | — | — | — | |
| 1.4762High-chromium · Chromium-aluminium-silicon | 1.4762X10CrAlSi25 / X10CrAl24 | — | — | — | |
| 446High-chromium · Heat-resistant ferritic | 1.4749X18CrN28 | 446 | S44600 | SUH446 | |
| 446 / X8Cr24Ferritic · High chromium | 1.4763X8Cr24 | 446 | S44600 | — | |
| 1.4713Ferritic · Heat resistantX10CrAl7 | 1.4713X10CrAlSi7 | — | — | — | |
Frequently asked questions
Which stainless steel is most heat resistant?
There is no single answer. 310S and 314 stand out with high chromium and nickel; 253 MA suits repeated heating, ferritic 1.4762 and 446 certain hot gases. The choice depends on gas composition, load and duration.
What is the difference between 309S and 310S?
310S is an austenitic heat-resisting steel with more chromium and nickel than 309S. Both are used in furnace parts.
Is heat-resistant stainless magnetic?
Austenitic 309S, 310S and 314 generally do not when annealed; ferritic 1.4742, 1.4762 and 446 are magnetic. This does not determine heat resistance.
Are oxidation resistance and creep strength the same?
No. Oxidation resistance describes surface protection in hot gas; creep strength describes hot metal keeping its shape under long-term load.
LET’S CLARIFY YOUR REQUIREMENT
Your next project.
The right starting point.
For European-origin material with an EN 10204 3.1 certificate, talk to our team directly about the supply options for your project.
Request a quote