- Grade / Alloy
- 50CrV4 / 51CrV4
- EN / W.Nr.
- 1.815951CrV4
- AISI / SAE
- 6150
- UNS
- —
- Other names
- 50CrV4 · JIS SUP10 · BS 735A51
- Family
- Alloy steel
- Density
- 7.85 g/cm³20 °C
1.8159 (50CrV4 / 51CrV4) chemical composition
Chemical composition
Composition limitsEN 10083-3 cast analysis limits for 51CrV4 (thyssenkrupp; Ovako’s EN 10089 values are the same).
| Element | Content (% by mass) |
|---|---|
| CCarbon | 0.47–0.55 |
| SiSilicon | ≤ 0.4 |
| MnManganese | 0.7–1.1 |
| PPhosphorus | ≤ 0.025 |
| SSulfur | ≤ 0.025 |
| CrChromium | 0.9–1.2 |
| VVanadium | 0.1–0.25 |
Values describe the grade, not the analysis of a specific batch. The applicable product specification and material certificate determine acceptance.
50CrV4 or 51CrV4?
Steel 1.8159 was called 50CrV4 in the former DIN 17200; in EN 10083-3 and EN 10089 its name is 51CrV4. The material number did not change, so both names describe the same steel and both are used in the market. The Saarstahl data sheet is headed “51CrV4 (50CrV4)”.
Chromium raises hardenability, while vanadium refines the grain and helps toughness after tempering. Saarstahl recommends it at 900–1200 MPa for machine and vehicle parts such as gears, pinions and shafts; Ovako describes its use as an EN 10089 spring steel in quenched-and-tempered springs.
50CrV4 mechanical properties (quenched and tempered, +QT)
The table gives the EN 10083-3 minimum values of quenched-and-tempered 51CrV4 by diameter range. Tempered lower for spring use, strength is much higher: with Ovako’s EN 10089 reference spring treatment (quench from 850 °C, temper at 450 °C) Rm is 1350–1650 MPa.
| Diameter d (mm) | Rp0.2 min (MPa) | Rm (MPa) | A min (%) | Z min (%) |
|---|---|---|---|---|
| ≤ 16 | 900 | 1100–1300 | 9 | 40 |
| 16–40 | 800 | 1000–1200 | 10 | 45 |
| 40–100 | 700 | 900–1100 | 12 | 50 |
| 100–160 | 650 | 850–1000 | 13 | 50 |
| 160–250 | 600 | 800–950 | 13 | 50 |
Sources and technical details
Thickness equivalents: ≤ 8, 8–20, 20–60, 60–100 and 100–160 mm. Charpy (ISO-V) at least 30 J. Saarstahl and thyssenkrupp give the same values.
Saarstahl — 51CrV4 (50CrV4) data sheet — Werkstoff-Datenblatt, p.1; EN 10083 quenched-and-tempered steel.
thyssenkrupp Materials Services — 51CrV4 / 1.8159 — Werkstoffdatenblatt, pp.1–2; references DIN EN 10083-3:2007.
Heat treatment, hardness and physical properties
Soft-annealed (+A) bar is at most 248 HB and should be ordered in this condition where shearability matters. Density is 7.85 kg/dm³ at 20 °C and the elastic modulus 212 GPa.
| Treatment or condition | Value | Note |
|---|---|---|
| Hardening | 820–860°C | In oil |
| Tempering (QT) | 540–680°C | In air |
| Soft annealing | 680–720°C | In furnace |
| Soft annealed (+A) | Max 248 HB | Saarstahl, thyssenkrupp, Ovako |
| Thermal expansion (20–100 °C) | 12.1 × 10⁻⁶ /K | thyssenkrupp |
Sources and technical details
Saarstahl — 51CrV4 (50CrV4) data sheet — Werkstoff-Datenblatt, p.1; EN 10083 quenched-and-tempered steel.
thyssenkrupp Materials Services — 51CrV4 / 1.8159 — Werkstoffdatenblatt, pp.1–2; references DIN EN 10083-3:2007.
50CrV4 equivalents: 6150, SUP10, 735A51
Saarstahl lists SAE 6150, BS 735A51 and AFNOR 50CrV4 as counterparts; Ovako lists AISI 6150. The Japanese spring-steel counterpart is SUP10. The counterparts have similar compositions, but limits and delivery conditions differ between standards, so the applicable standard should be stated when ordering.
Typical application areas
Gears, pinions, shafts, leaf and coil springs.