- Grade / Alloy
- 41Cr4
- EN / W.Nr.
- 1.703541Cr4
- AISI / SAE
- 5140
- UNS
- —
- Other names
- 41CrS4 (1.7039) · JIS SCr440
- Family
- Alloy steel
- Density
- 7.8 g/cm³
1.7035 (41Cr4) chemical composition
Chemical composition
Composition limitsEN 10083-3 cast analysis limits for 41Cr4 (Ovako and EN tables); 41CrS4 has 0.020–0.035 sulphur.
| Element | Content (% by mass) |
|---|---|
| CCarbon | 0.38–0.45 |
| SiSilicon | ≤ 0.4 |
| MnManganese | 0.6–0.9 |
| PPhosphorus | ≤ 0.025 |
| SSulfur | ≤ 0.035 |
| CrChromium | 0.9–1.2 |
Values describe the grade, not the analysis of a specific batch. The applicable product specification and material certificate determine acceptance.
41Cr4 in drive components
41Cr4 is a chromium-alloyed quenched-and-tempered steel: it is hardened and then reheated in a controlled way (tempering). The producer data sheet recommends it, at a tensile strength of 800–1100 MPa in this condition, for drive components such as crankshafts, front axles, steering knuckles and steering parts.
Without molybdenum it does not harden as deeply as 42CrMo4 (4140); Ovako states that it through-hardens in oil up to about 40 mm diameter. It is therefore used for parts of moderate section needing less strength than 42CrMo4. Its surface can be induction hardened to at least 52 HRC.
41Cr4 mechanical properties (quenched and tempered, +QT)
The strength of quenched-and-tempered 41Cr4 falls as the section grows, because the core of a thick part does not cool as quickly. The table gives the EN 10083-3 minimum values by diameter range; no values are given above 100 mm.
| Diameter d (mm) | Rp0.2 min (MPa) | Rm (MPa) | A min (%) | Z min (%) |
|---|---|---|---|---|
| ≤ 16 | 800 | 1000–1200 | 11 | 30 |
| 16–40 | 660 | 900–1100 | 12 | 35 |
| 40–100 | 560 | 800–950 | 14 | 40 |
Sources and technical details
Thickness equivalents: ≤ 8, 8–20 and 20–60 mm. Charpy (ISO-V) at least 30–35 J. Ovako gives the same values for the 16–40 and 40–100 mm ranges.
Saarstahl — 41Cr4 / 41CrS4 data sheet — Werkstoff-Datenblatt, p.1; EN 10083 quenched-and-tempered steel.
Ovako Steel Navigator — 41Cr4 — Composition, mechanical property and heat-treatment tables.
Heat treatment and delivery hardness
Bar is usually supplied soft annealed (+A) or treated for shearability (+S) and quenched and tempered after machining. The temperatures below are processing temperatures, not service temperatures.
| Treatment or condition | Value | Note |
|---|---|---|
| Hardening | 820–860°C | Oil or water |
| Tempering | 540–680°C | To the required strength |
| Soft annealing | 680–720°C | Slow furnace cooling |
| Soft annealed (+A) | Max 241 HB | Saarstahl and Ovako |
| Treated for shearability (+S) | Max 255 HB | Saarstahl |
Sources and technical details
Saarstahl — 41Cr4 / 41CrS4 data sheet — Werkstoff-Datenblatt, p.1; EN 10083 quenched-and-tempered steel.
Ovako Steel Navigator — 41Cr4 — Composition, mechanical property and heat-treatment tables.
41Cr4 equivalents: 5140, SCr440, 530M40
41Cr4 has the material number 1.7035; its resulphurised free-machining version is 41CrS4 (1.7039). Saarstahl lists SAE 5140, BS 530M40 and AFNOR 42C4 as counterparts; the Japanese counterpart is SCr440. These are close, not identical: SAE 5140 has 0.70–0.90 chromium, 41Cr4 0.90–1.20.
Typical application areas
Crankshafts, axles, steering knuckles, steering parts, shafts.