PRECISION IN MATERIAL. CLARITY IN SUPPLY.

ALLOY STEEL

1.7218 (25CrMo4) Alloy Steel

25CrMo4 (1.7218) is a low-carbon chromium-molybdenum quenched-and-tempered steel and the close counterpart of SAE 4130. Its high toughness and good weldability suit axles, steering knuckles and turbine parts in automotive and aircraft engineering. This page covers the 1.7218 material properties: chemical composition, mechanical values and applications.

Grade / Alloy
25CrMo4
EN / W.Nr.
1.721825CrMo4
AISI / SAE
4130
UNS
—
Other names
25CD4 · BS 708A25
Family
Alloy steel
Density
7.8 g/cm³

1.7218 (25CrMo4) chemical composition

Chemical composition

Composition limits

EN ISO 683-2 / EN 10083-3 composition limits for 25CrMo4 (Ovako).

25CrMo4 — chemical composition, % by mass
ElementContent (% by mass)
CCarbon0.22–0.29
SiSilicon≤ 0.4
MnManganese0.6–0.9
PPhosphorus≤ 0.025
SSulfur≤ 0.035
CrChromium0.9–1.2
MoMolybdenum0.15–0.3

Values describe the grade, not the analysis of a specific batch. The applicable product specification and material certificate determine acceptance.

25CrMo4 where toughness and welding matter

25CrMo4 is a chromium-molybdenum quenched-and-tempered steel with low carbon. Saarstahl describes good welding properties at a tensile strength of 700–950 MPa and use in automotive and aircraft parts needing high toughness, such as axles, steering knuckles, turbine parts and turbine rotors.

Low carbon reduces the risk of hardening during welding, but welding still needs preheating and a suitable procedure; Ovako describes it as weldable under certain conditions. Thick parts needing higher strength use 42CrMo4 (4140).

25CrMo4 mechanical properties (quenched and tempered, +QT)

The minimum values of quenched-and-tempered 25CrMo4 depend on diameter: as the section grows, yield and tensile strength fall and elongation rises. The table shows the EN 10083-3 values.

Diameter d (mm)Rp0.2 min (MPa)Rm (MPa)A min (%)Z min (%)
≤ 16700900–11001250
16–40600800–9501455
40–100450700–8501560
100–160400650–8001660
Sources and technical details

Thickness equivalents: ≤ 8, 8–20, 20–60 and 60–100 mm. Charpy (ISO-V) at least 45–50 J. Ovako’s 25–160 mm bar values give the same yield, tensile and elongation limits.

Saarstahl — 25CrMo4 data sheet — Werkstoff-Datenblatt, p.1; EN 10083 quenched-and-tempered steel.

Ovako Steel Navigator — 25CrMo4 — Composition, mechanical property and heat-treatment tables.

Heat treatment and delivery hardness

The values below are processing temperatures from the producer data sheets. For water quenching Ovako recommends a lower temperature (820–850 °C).

Treatment or conditionValueNote
Hardening840–880°CWater or oil
Tempering540–680°CAir cooling
Normalising860–890°CIn air
Soft annealed (+A)Max 212 HBSaarstahl
Treated for shearability (+S)Max 255 HBSaarstahl
Sources and technical details

Saarstahl — 25CrMo4 data sheet — Werkstoff-Datenblatt, p.1; EN 10083 quenched-and-tempered steel.

Ovako Steel Navigator — 25CrMo4 — Composition, mechanical property and heat-treatment tables.

Are 25CrMo4 and 4130 the same steel?

Saarstahl and Ovako give SAE 4130 as the counterpart of 25CrMo4; the British counterpart is BS 708A25 and the French one 25CD4. They are close, not identical: SAE 4130 has 0.28–0.33 carbon and 0.80–1.10 chromium, while 25CrMo4 has 0.22–0.29 carbon and 0.90–1.20 chromium. A project specifying 4130 should check the composition and mechanical values of the EN material separately.

Typical application areas

Axles, steering knuckles, turbine parts, welded structural parts.

Product and cutting options

Relevant product forms for this material are listed below. Availability varies with grade and dimensions.