HARDNESS CONVERSION
HRC to HB conversion chart
Convert HRC to an approximate HB value, or the other way round. Choose the material group; HRC – HB tables for steel and stainless follow below.
MEASURED HARDNESS
Scale and value
Table range: 20.5–57 HRC. A decimal comma or point is accepted.
Approximate comparison for stainless steels. Not a grade-specific measurement.
Table scope
Uses a general stainless steel comparison dataset. Grade and material condition can affect the relationship within this group. It does not apply to another metal family.
HARDNESS COMPARISONS
Approximate conversion
45
Your input—
No table comparison≈422
Approximate comparison≈448
Approximate comparisonEstimated tensile strength
UTS · N/mm² (MPa)
≈ 1447 N/mm²
A material-dependent estimate; not a replacement for a tensile test or certificate result.
HRC: 45 HRB: — HB: ≈ 422 HV: ≈ 448 Estimated tensile strength (UTS): ≈ 1447 N/mm²
Hardness conversion tableHRC · HRB · HB · HV · Estimated UTS
The selected row, or two adjacent rows used in calculation, are highlighted. A dash indicates an unavailable comparison.
| HRCRockwell C | HRBRockwell B | HBBrinell | HVVickers | UTSEstimated · N/mm² |
|---|---|---|---|---|
| 57 | — | — | 640 | — |
| 56 | — | — | 615 | — |
| 54.5 | — | — | 591 | — |
| 53.5 | — | — | 569 | — |
| 52 | — | — | 547 | — |
| 51 | — | — | 528 | — |
| 49.5 | — | — | 508 | — |
| 48.5 | — | — | 491 | 1539 |
| 47 | — | 444 | 474 | 1520 |
| 45.5 | — | 429 | 455 | 1471 |
| 44.5 | — | 415 | 440 | 1422 |
| 43 | — | 401 | 425 | 1363 |
| 42 | — | 388 | 410 | 1314 |
| 40.5 | — | 375 | 396 | 1265 |
| 39 | — | 363 | 383 | 1236 |
| 38 | — | 352 | 372 | 1187 |
| 36.5 | — | 341 | 360 | 1157 |
| 35.5 | — | 331 | 350 | 1118 |
| 34.5 | — | 321 | 339 | 1089 |
| 33 | — | 311 | 328 | 1049 |
| 32 | — | 302 | 319 | 1020 |
| 31 | — | 293 | 309 | 990 |
| 30 | — | 285 | 301 | 971 |
| 29 | — | 277 | 292 | 941 |
| 27.5 | — | 269 | 284 | 912 |
| 26.5 | — | 262 | 276 | 892 |
| 25.5 | 100 | 255 | 269 | 873 |
| 24 | 99 | 248 | 261 | 853 |
| 23 | 98 | 241 | 253 | 824 |
| 22 | 97 | 235 | 247 | 794 |
| 20.5 | 96 | 229 | 241 | 775 |
| — | — | 223 | 235 | 755 |
| — | 95 | 217 | 228 | 745 |
| — | 94 | 212 | 223 | 716 |
| — | 93 | 207 | 218 | 696 |
| — | 91 | 197 | 208 | 667 |
| — | 89 | 187 | 197 | 637 |
| — | 87 | 179 | 189 | 608 |
| — | 85 | 170 | 179 | 559 |
| — | 83 | 163 | 172 | 539 |
| — | 81 | 156 | 165 | 530 |
| — | 79 | 149 | 157 | 500 |
| — | 77 | 143 | 150 | 481 |
| — | 74 | 137 | 144 | 471 |
| — | 72 | 131 | 138 | 461 |
| — | 69 | 126 | 133 | 451 |
| — | 67 | 121 | 127 | 431 |
| — | 64 | 116 | 122 | 422 |
| — | 61 | 111 | 117 | 402 |
| — | — | 107 | 113 | 382 |
| — | — | 103 | 108 | 373 |
Sources and technical details
Numerical table source: BSSA — stainless steel hardness comparison. The source defines the scope of the approximate comparison; it is not a test result for a particular component.
HRC to HB conversion chart
Rows are the measured comparison points the calculator uses, read in both directions: find HRC in the first column for HB, or HB in the second column for HRC. Values between rows are interpolated by the calculator above.
HRC – HB: carbon and low-alloy steelapproximate; reference points of the calculator
| HRC | HB |
|---|---|
| 46.9 | 447 |
| 46.1 | 437 |
| 45.3 | 428 |
| 44.5 | 418 |
| 43.6 | 409 |
| 42.7 | 399 |
| 41.8 | 390 |
| 40.8 | 380 |
| 39.8 | 371 |
| 38.8 | 361 |
| 37.7 | 352 |
| 36.6 | 342 |
| 35.5 | 333 |
| 34.4 | 323 |
| 33.3 | 314 |
| 32.2 | 304 |
| 31 | 295 |
| 29.8 | 285 |
| 29.2 | 280 |
| 28.5 | 276 |
| 27.8 | 271 |
| 27.1 | 266 |
| 26.4 | 261 |
| 25.6 | 257 |
| 24.8 | 252 |
| 24 | 247 |
| 23.1 | 242 |
| 22.2 | 238 |
| 21.3 | 233 |
| 20.3 | 228 |
HRC – HB: stainless steelapproximate; reference points of the calculator
| HRC | HB |
|---|---|
| 47 | 444 |
| 45.5 | 429 |
| 44.5 | 415 |
| 43 | 401 |
| 42 | 388 |
| 40.5 | 375 |
| 39 | 363 |
| 38 | 352 |
| 36.5 | 341 |
| 35.5 | 331 |
| 34.5 | 321 |
| 33 | 311 |
| 32 | 302 |
| 31 | 293 |
| 30 | 285 |
| 29 | 277 |
| 27.5 | 269 |
| 26.5 | 262 |
| 25.5 | 255 |
| 24 | 248 |
| 23 | 241 |
| 22 | 235 |
| 20.5 | 229 |
Worked examples
- 30 HRC → ≈ 287 HB in carbon steel, ≈ 285 HB in stainless.
- 40 HRC → ≈ 373 HB in carbon steel, ≈ 371 HB in stainless.
What are HRC and HB?
HRC (Rockwell C) is read from the depth of indentation of a 120° diamond cone under a 150 kgf total load; it is used for hardened steels and tool steels.
HB (Brinell) is calculated from the diameter of the impression of a hard metal ball (for steels usually 10 mm and 3000 kgf); its large impression gives an average value on castings and coarse structures. With a hard metal ball the result is also written HBW.
How do you convert HRC to HB?
There is no exact formula between HRC and HB; the two tests use different indenters and loads. Conversion uses comparison tables measured on both scales for the same material group. A value on a table row is read directly; one between two rows is interpolated between those rows only.
The result is approximate and depends on the material group. For acceptance or certificates, measure the required scale directly.
Valid range of the chart
The carbon and low-alloy steel chart covers 20.3–46.9 HRC and 228–447 HB; the stainless steel chart covers 20.5–47 HRC and 229–444 HB. No conversion is given outside these ranges.
Frequently asked questions
What is 45 HRC in HB?
About 424 HB for carbon and low-alloy steel and about 422 HB for stainless steel. The value is approximate and depends on the material group.
What is 424 HB in HRC?
About 45 HRC for carbon and low-alloy steel and about 45.1 HRC for stainless steel. The reverse conversion reads the same comparison table.
Is there a formula from HRC to HB?
There is no universal formula. Conversion relies on comparison tables measured on both scales for the same material group, and the tables differ by material.
Is the HRC to HB conversion the same for stainless?
Not exactly; each material group has its own chart. For 45 HRC: about 424 HB for carbon and low-alloy steel and about 422 HB for stainless steel. Choose the material group in the calculator.
What is the difference between HRC and HB?
HRC (Rockwell C) is read from the depth of indentation of a 120° diamond cone under a 150 kgf total load; it is used for hardened steels and tool steels. HB (Brinell) is calculated from the diameter of the impression of a hard metal ball (for steels usually 10 mm and 3000 kgf); its large impression gives an average value on castings and coarse structures. With a hard metal ball the result is also written HBW.